Chemical Composition And Mechanical Properties of Steel (Indian Standard)
|
IS : 10748 - Specification Of Hot Rolling
Steel Strips For Welded Tubes & Pipe |
CHEMICAL COMPOSITION |
| Grade |
C%
Max |
Mn
% Max. |
S% Max. |
P%
Max. |
| I |
0.10 |
0.50 |
0.05 |
0.05 |
| II |
0.12 |
0.60 |
0.05 |
0.05 |
| III |
0.16 |
1.20 |
0.05 |
0.05 |
| IV |
0.20 |
1.30 |
0.05 |
0.05 |
| V |
0.25 |
1.30 |
0.05 |
0.05 |
MECHANICAL PROPERTIES |
| Grade |
UTS
( Min.) Mpa |
YS
( Min.) Mpa |
EI. % ( Min. ) 5.65 Sqrt (So) |
| I |
290 |
170 |
30 |
| II |
330 |
210 |
28 |
| III |
410 |
240 |
25 |
| IV |
430 |
275 |
20 |
| V |
490 |
310 |
15 |
|
IS : 6240 HR - Steel Plate, Sheet and Coil
for LP |
| CHEMICAL COMPOSITION |
| Constituent |
Percent |
| Carbon, Max. |
0.16 |
| Manganese, Min |
0.30 |
| Silicon, Max. |
0.25 |
| Sulphur, Max. |
0.030 |
| Phosphorous, Max. |
0.030 |
| Aluminium, Min |
0.02 |
| MECHANICAL
PROPERTIES |
| Property |
Grade
* |
| Tensile Strength Mpa
(kgf/mm²) |
350 to 450 ( 36 to
46 ) |
| Yield Strength. Mpa ( Kg/mm²)
Min |
240 (25) |
| Elongation, Min percent on guage
length 5.65 OSo |
25 |
| Bend |
t |
| EC v ( for 2.80-3.15 mm
thickness) min |
13.5 |
| * Both longitudinal
and transverse directions. |
|
TOLERANCE AS PER IS : 513 |
Tolerance on Thickness of Sheets |
| |
Tolerance on the
thickness for different width |
Nominal
Thickness |
Upto
1250
mm |
Above
1250
Upto 1600 |
Above
1600 |
| Upto 0.25 |
+/-
0.03 |
- |
- |
| Above 0.25-0.40 |
+/-
0.04 |
- |
- |
| Above 0.40-0.60 |
+/-
0.05 |
+/-
0.06 |
- |
| Above 0.60-0.80 |
+/-
0.06 |
+/-
0.07 |
+/-
0.08 |
| Above 0.80-1.00 |
+/-
0.08 |
+/-
0.09 |
+/-
0.10 |
| Above 1.00-1.25 |
+/-
0.09 |
+/-
0.10 |
+/-
0.12 |
| Above 1.25-1.60 |
+/-
0.11 |
+/-
0.12 |
+/-
0.14 |
| Above 1.60-2.00 |
+/-
0.12 |
+/-
0.14 |
+/-
0.16 |
|
Tolerance on Width Of
Sheets |
| Width of Sheets |
Tolerance |
| Upto 1250 mm |
+7 |
-0 |
| Above 1250 mm |
+10 |
-0 |
|
Tolerance on Length of Sheets |
| Length |
Tolerance |
| Upto
2000 mm |
+15 |
-0 |
| Above
2000 mm |
+0.75
% of the length |
-0 |
|
Chamfer Tolerance For Coils and Cut Length |
| Form |
Tolerance |
| Coil
|
20
mm in any 5000 mm length |
| Cut
Length |
0.4%
X length |
|
Standard Flatness Tolerance for cut lengths |
| Thickness
|
Tolerance
on specified width |
| Upto
1200 |
Above
1200 - Upto 1500 |
Above
1500 |
| Upto 0.63 |
15 |
18 |
22 |
| Above 0.63-1.25 |
12 |
15 |
19 |
| Above 1.25 |
10 |
12 |
17 |
|
Special Flatness Tolerance for
Cut lengths Roller Levelled and Stretcher Levelled |
| Thickness
|
Tolerance on specified width |
| Upto
1200 |
Above
1200 Upto 1500 |
Above
1500 |
| Upto 0.63 |
6 |
7 |
8 |
| Above 0.63-1.25 |
5 |
6 |
7 |
| Above 1.25 |
4 |
5 |
6 |
|
|
IS : 2062 - Specification of Steel for General Structural Purposes |
| CHEMICAL COMPOSITION |
| Grade
|
C%
Max. |
Mn%
Max. |
S%
Max. |
P%
Max. |
Si%
Max. |
C.E.%
Max. |
| A |
0.23 |
1.50 |
0.050 |
0.050 |
0.40 |
0.42 |
| B |
0.22 |
1.50 |
0.045 |
0.045 |
0.40 |
0.41 |
| C |
0.20 |
1.50 |
0.040 |
0.040 |
0.40 |
0.39 |
| MECHANICAL PROPORTIES |
| Grade |
UTS(MPa)
Min. |
Y.S.(MPa)
Min. |
El.%
Min. 5.65 Sqrt(So) |
Bend
Test |
| A |
410 |
250 |
240 |
230 |
23 |
3T |
| B |
410 |
250 |
240 |
230 |
23 |
2T & 3T * |
| C |
410 |
250 |
240 |
230 |
23 |
2T |
* 2T - <=
25mm
* 3T - > 25mm |
|
| IS : 3039 -
Specification of Structural Steel for Ship Building |
| CHEMICAL COMPOSITION |
| Grade
|
C% Max. |
Mn% |
S%
Max. |
P% Max. |
Si% Max. |
Al%
Min. |
| I |
0.23 |
* |
0.040 |
0.040 |
** |
0.01 |
| II |
0.21 |
0.70-1.4 |
0.040 |
0.040 |
0.10-0.35 |
- |
| III |
0.18 |
0.70-1.5 |
0.040 |
0.040 |
0.19-0.50 |
0.015 |
| MECHANICAL PROPERTIES |
| Grade |
UTS (MPa) |
Y.S. (MPa) Min. |
EI.% Min.
5.65 Sqrt (So) |
| < 25 mm. |
> 25 < 50 mm. |
| I |
400-490 |
230 |
220 |
22 |
| II |
400-900 |
235 |
235 |
22 |
| III |
400-490 |
235 |
235 |
22 |
|
| IS :
1786 - High Strength Deformed Steel Bars and Wires for Concrete Reinforcement
|
| CHEMICAL COMPOSITION |
Constituent |
Percent, Maximum |
SAIL-TMT(Fe 415/FE 500/Fe 550) |
| |
SAIL
TMT
415 |
Fe 415
|
SAIL
TMT 500 |
Fe 500 |
SAIL
TMT
550 |
Fe 500 |
|
| Carbon |
0.25 |
0.30 |
0.25 |
0.30 |
0.25 |
0.30 |
0.20 |
| Sulphur |
0.05 |
0.06 |
0.05 |
0.055 |
0.05 |
0.055 |
0.045 |
| Phosphorus |
0.05 |
0.06 |
0.05 |
0.055 |
0.05 |
0.050 |
0.045 |
| Sulphur and Phosphorus |
0.10 |
0.11 |
0.10 |
0.105 |
0.10 |
0.10 |
0.09 |
| Corrosion Resistant
Elements |
- |
- |
- |
- |
- |
- |
0.75 min |
| Carbon Equivalent |
- |
- |
- |
- |
- |
- |
0.53 max |
| MECHANICAL PROPERTIES |
| Property |
Grade |
| |
Fe
415 |
SAIL
TMT
415 |
Fe
500 |
SAIL
TMT
500 |
Fe
550 |
SAIL
TMT
550 |
| 0.2 percent proof
stress/yield stress Min N/mm.sq. |
415 |
415 |
500 |
500 |
550 |
550 |
| Elongation.percent ,Min,on
gauge length 5.65.Square Root(A) where A is the cross-sectional area of the test piece |
14.5 |
22(Up to 28mm dia) 20
(Above 28 mm dia) |
12 |
20(Up to 28mm dia) 18
(Above 26 mm dia) |
8 |
18(Upto 25 mm
dia) 16(Above 28 mm dia) |
| Tensile
Strength,Min. |
10%
more than the actual 0.2% proof stress but not less than 48.5 N/mm.sq. |
10%
more than the actual 0.2% proof stress but not less than 500 N/mm.sq. |
8%
more than actual 0.2% proof stress but not less than 545 N/mm.sq. |
8% more than the
actual 0.2% proof stress but not less than 580 N/mm.sq.
(Upto 28mm dia) & 560 N/mm.sq.)
(above 28 mm dia) |
6%
more than the actual
0.2% proof
stress but not less than 585 N/mm.sq. (Upto
28mm dia) & 560 N/mm.sq.)
(above 28 mm dia) |
6% more than the actual
0.2% proof
stress but not less than 630 N/mm.sq.
(Upto 28mm dia)
& 610 N/mm.sq.(above 28 mm dia)
Upto 28mm dia) & 560 N/mm.sq.)
(above 28 mm dia) |
|
SPECIFICATION FOR WIRE RODS |
| Specifications |
Grade |
Chemical Composition |
Mechanical Properties |
| %C |
%Mn |
%S |
%P |
Yield
Mpa |
Tensile
Mpa |
Elongation
% |
Structure Quality
Wire Rods |
IS2062
Grade A |
0.23
max |
1.50
max |
0.05
max |
0.50
max |
250
min |
410
min |
23
min |
Drawing Quality
Wire Rods |
SWR-14 |
0.14
max
0.08-013 |
0.60
max
0.30-0.60 |
0.05
max
0.05 max |
0.05
max
0.04 max |
- |
- |
- |
Low Carbon Drawing
Quality Wire Rods |
SWR-10
SAE-1008 |
0.1
max
0.1 max |
0.6
max
0.3 max |
0.04
max
0.05 max |
0.04
max
0.04 max |
- |
- |
- |
Electrode Quality
Wire Rod |
IS-2879
Rimming Grade |
0.1
max |
0.38-0.62 |
0.03
max |
0.03
max |
- |
- |
- |
|
IS:1079-Specification of Hot Rolled Carbon Steel
Sheets & Strips |
CHEMICAL COMPOSITION |
| Grade |
C%
Max |
Mn %
Max |
S%
Max |
P%
Max |
| O |
0.15 |
0.60 |
0.055 |
0.055 |
| D |
0.12 |
0.50 |
0.04 |
0.04 |
| DD |
0.10 |
0.45 |
0.035 |
0.035 |
| EDD |
0.08 |
0.40 |
0.030 |
0.03 |
MECHANICAL PROPERTIES |
| Grade |
UTS
MPa |
YS(Min.)
MPa |
EI.% Min.
Lo-80 mm b-20 mm |
| O |
- |
- |
- |
| D |
- |
- |
28 |
| DD |
260-390 |
- |
32 |
| EDD |
260-380 |
- |
36 |
|
Specification |
Chemical composition (max) |
Mechanical Properties |
| |
C |
Mn |
S |
P |
Tensile
Strength
Min. Mpa |
Yield
Strength
Min. Mpa |
% Elongation
guage
length
5.65 So |
Nb+V+T |
| IS-2062
Gr A (SK) |
0.23 |
1.5 |
0.050 |
0.050 |
410 |
240 |
23 |
0.20 |
| IS-2062
Gr B (SK) |
0.20 |
1.5 |
0.045 |
0.045 |
410 |
240 |
23 |
. |
| SAIL-MA
300 |
0.25 |
1.5 |
0.055 |
0.055 |
440-560 |
300 |
20 |
Maximum
for all |
| SAIL-MA
300 HI |
0.20 |
1.5 |
0.040 |
0.040 |
440-560 |
300 |
21 |
| SAIL-MA
350 |
0.25 |
1.5 |
0.040 |
0.040 |
490-610 |
350 |
20 |
| SAIL-MA
350 HI |
0.20 |
1.5 |
0.040 |
0.040 |
540-660 |
410 |
19 |
. |
| SAIL-MA
410 |
0.25 |
1.5 |
0.040 |
0.040 |
540-660 |
410 |
20 |
. |
|